How to 3D print a part, from file to finished print

A practical walkthrough of 3D printing for beginners and anyone printing products. Get a model, slice it, print it, finish and check the part, and fix the common failures.

By Printlooper Team · Published · 23 min read

Key takeaways

  • Many failed prints start before the printer moves, so check the mesh, the units and the orientation before you slice.
  • Strength comes mostly from walls, not infill. Three to four walls with 20 to 40% infill suits most functional parts.
  • Start PLA around 205 to 215 °C with a 55 to 60 °C bed and PETG around 230 to 250 °C with a 70 to 90 °C bed, then tune inside the filament maker's range.
  • Watch the whole first layer every time. Lines should be slightly flattened and touching, with no gaps and no ridges.
  • Resin printing needs nitrile gloves, ventilation and waste handling that follows the safety data sheet and local rules, and that includes water-washable resin.
  • No printer? Upload the file on Printlooper and compare all-in prices from independent print shops that ship to US addresses.

This guide takes a part from a file to a finished, checked print. It is for first-time printers, designers who want files that print well on other people's machines, sellers who need every unit to match, and print shops that want a shared checklist.

You will get and repair a model, choose a process and material, orient the part, set up the slicer (the program that turns a model into printer instructions), print, finish, check the result and fix the common failures. The numbers are starting points for a 0.4 mm nozzle, to tune with your filament maker's range and a few calibration prints.

No printer? Read the first three sections, then skip to the section on ordering a print.

Get a printable model

Every print starts as a 3D model, usually an STL or 3MF file. STL holds surface triangles only. 3MF can also carry units, colors, several parts and slicer settings, and STL vs 3MF compares them. There are four ways to get a model.

Design it

Fusion, Onshape and FreeCAD suit functional parts with exact dimensions. Blender suits sculpted and organic shapes. Model in millimeters, and read designing for 3D printing before you model anything that has to fit.

Download it, and check the license

The license decides what you can do with the print. A Creative Commons license with NC (NonCommercial) in its name rules out uses mainly aimed at commercial advantage or payment, which covers selling prints. Some designers sell a separate commercial license. If the license does not clearly allow selling prints, assume it does not and ask.

Generate it

The AI 3D model generator turns a typed description into a printable model. Treat the result as a prototype, since a print can differ from the preview and generated shapes are not exact-fit parts. To sell prints of a generated model on Printlooper, it must be one closed piece, and it sells only as a printed product in your own store, not on the designer marketplace.

Request it

When the part does not exist yet, request a design. You post a brief, designers reply with scope and price, and you pick one. Community requests are listed on the requests board. Include sizes in millimeters, the parts it must fit, photos with a ruler in frame, the material and the quantity.

Check and repair the mesh

A slicer can only build a solid it understands. Check four things before slicing.

  • Watertight. The surface is closed with no holes, so the slicer can tell inside from outside.
  • Manifold. Every edge is shared by exactly two faces. Non-manifold edges confuse the slicer and cause missing layers.
  • Normals. Every face points outward. Flipped faces make part of the model read as inside out.
  • Units and scale. STL files carry no units. A part modeled in inches imports 25.4 times too small in a millimeter slicer, and one exported in meters 1,000 times too small. Check the bounding box first.

Most slicers, including PrusaSlicer, Bambu Studio, OrcaSlicer and Cura, fix simple errors on import. For the rest, Blender's 3D Print Toolbox and Meshmixer's Inspector find holes, non-manifold edges and thin walls. Repair the source file and export again when you can, because a patched STL drifts away from the design.

Then slice and scrub through the layer preview. On a 0.4 mm nozzle, walls under about 0.8 mm (two extrusion lines) print weak, and features thinner than one line can vanish. If a feature disappears in the preview, it disappears in the print.

Mesh check before slicing

  • Bounding box matches the intended size in millimeters
  • No holes or open edges reported by the slicer or repair tool
  • No non-manifold edges or flipped normals
  • Walls at least two line widths thick, 0.8 mm on a 0.4 mm nozzle
  • Parts meant to print as one are joined, and moving parts have clearance
  • Layer preview shows every wall, pin and text feature you expect

If you upload designs to Printlooper, every file gets a geometry check. It rejects a file when more than half its edges are non-manifold, or when more than 10% of its edges are open and it encloses no volume. Nothing is repaired for you, so fix the mesh first, as preparing an STL or 3MF for upload explains.

Choose a process and material

Three processes cover nearly all consumer and small-business printing. FDM (fused deposition modeling) melts plastic filament and lays it down line by line. Resin printing (SLA, DLP and LCD) cures liquid resin with light, one thin layer at a time. SLS and MJF fuse nylon powder with a laser, or with a fusing agent and heat.

How the three main processes compare
ProcessBest forTypical layer heightWatch out for
FDM (filament)Functional parts, large parts, props and everyday products0.12 to 0.28 mmVisible layer lines, weaker between layers, supports under steep overhangs
Resin (SLA, DLP, LCD)Miniatures, jewelry and small detailed parts0.025 to 0.05 mmSmall build volume, brittle standard resins, skin-irritating uncured resin, wash and cure steps
SLS and MJF (nylon powder)Tough functional parts and small production runsAbout 0.08 to 0.12 mmProfessional machines, so parts usually come from a print service, slightly grainy surface, mostly white, gray or dyed black

FDM vs resin vs SLS goes deeper on processes, and the 3D printing materials guide covers PLA, PETG, ABS, ASA, TPU, nylon and resin. The short version for FDM is PLA for indoor parts that do not get hot or take impacts, PETG for functional parts, and ASA for parts that live outside.

Orient the part and plan supports

Orientation decides strength, surface quality, support use and print time, so settle it first.

Orientation on FDM printers

  • Strength runs along the layers. FDM parts are weakest between layers, so a wall hook printed standing up snaps at a layer line. Print it on its side so the load runs along the lines.
  • Put the largest flat face on the bed, unless that face is the one people see.
  • Overhangs up to about 45 degrees from vertical print without support. Anything flatter needs support or a design change, such as a chamfer in place of a flat ledge.
  • Bridges (flat spans between two supports) print cleanly when short and sag as they get longer. Print a bridge test to find your printer's limit.
  • Horizontal holes droop at the top, so model them as teardrops or drill them out afterward.
  • Seams mark where each layer starts and ends. Put them on a back corner or a hidden edge.

Supports

Normal (grid) supports leave a flat underside. Tree or organic supports use less material and break away more cleanly from figures and curved shapes. Three settings matter most.

  • Overhang threshold, the angle past which the slicer adds support. Some slicers measure it from vertical and some from horizontal, so read the tooltip.
  • Top Z distance, the gap between support and part. About one layer height (0.2 mm at 0.2 mm layers) is a common start. Raise it if supports fuse to the part, and lower it if the underside sags.
  • Interface layers, two to four dense layers on top of the support for a smoother underside that peels off in one piece.

Block supports from faces that do not need them. Every support scar is sanding work later.

Orientation on resin printers

Tilt resin parts so each layer has a smaller cross-section and peels off the clear film at the bottom of the vat more easily, and avoid large flat faces parallel to the build plate. Hollow big parts to save resin, with walls thick enough not to be fragile, and add at least two drain holes, one close to the build plate, so trapped resin and air escape. Put supports on faces nobody sees.

Slicer settings explained

The slicer turns the model into G-code, the line-by-line instructions the printer follows. Start from the stock profile for your printer and filament, and change only what the part needs.

Inside an FDM part. Walls and top and bottom layers carry most of the strength; infill supports the inside.

Layer height and line width

Layer height is the thickness of each layer. Thinner layers give smoother curves, and halving the layer height roughly doubles print time. Prusa's guidance is to stay below 80% of the nozzle diameter (0.32 mm on a 0.4 mm nozzle), or layers bond poorly. Line width is how wide each extruded line is, and a little wider than the nozzle gives stronger walls.

Walls, top and bottom layers

Walls (also called perimeters) are the outlines of each layer, and they carry most of the load. One more wall usually adds more strength than doubling the infill. Top and bottom layers close the part. Aim for about 0.8 to 1.0 mm of top skin, or sparse infill shows through as gaps.

Infill

Infill is the internal structure. Gyroid supports the part well in every direction. Grid is fast. Lightning only holds up the top surfaces and adds almost no strength, so keep it for display pieces.

Adhesion: skirt, brim and raft

A skirt is a loop that primes the nozzle before the part starts. A brim is a flat ring attached to the first layer that holds down corners on tall, narrow or warp-prone parts, then peels off. A raft prints a full base under the part, and modern textured beds rarely need one.

Temperature, speed and cooling

Start in the middle of the spool's temperature range and tune with a temperature tower, a test print that changes temperature every few millimeters. Speed is limited by how fast the hotend melts plastic, measured as volumetric flow, roughly layer height x line width x speed. At 0.2 x 0.45 mm and 100 mm/s that is about 9 mm³/s. Prusa rates older E3D V6 style hotends at about 8 to 12 mm³/s and its Nextruder at 15 to 20, so check yours. PLA wants full cooling after the first layers. PETG wants much less, or its layers bond poorly.

Retraction

Retraction pulls filament back during travel moves so the nozzle does not ooze. Direct-drive extruders, with the motor on the print head, need far less than Bowden setups, which push filament through a long tube. Too much retraction grinds filament and causes clogs.

Starting values for PLA and PETG on a 0.4 mm nozzle. Tune within the filament maker's range.
SettingPLA startPETG startTune with
Layer height0.2 mm (0.12 to 0.28 mm)0.2 mm (0.12 to 0.28 mm)Detail versus print time
Line width0.42 to 0.45 mm0.42 to 0.45 mmWall strength and surface
Walls2 for display, 3 to 4 for functional parts3 to 4Load test on a sample part
Top and bottom layers5 top, 4 bottom5 top, 4 bottomGaps in the top surface
Infill10 to 15% for display, 20 to 40% for functional parts, gyroid or grid20 to 40% gyroidPart weight and strength
Support thresholdSupport past 45 to 50 degrees from verticalSame, and widen the top gap if supports fuseOverhang test print
AdhesionSkirt, plus a 3 to 5 mm brim on small or tall partsSkirt, plus a 5 mm brim on sharp cornersCorner lift
Nozzle temperatureMiddle of the maker's range, often 205 to 215 °CMiddle of the maker's range, often 230 to 250 °CTemperature tower
Bed temperature55 to 60 °C70 to 90 °CFirst layer adhesion and warping
First layer speed20 to 30 mm/s, or the stock profile20 to 30 mm/s, or the stock profileFirst layer appearance
Outer wall speedStock profile, or 40 to 60 mm/s on older printersStock profile, or 30 to 50 mm/s on older printersSurface finish and ringing
Inner walls and infillUp to the hotend's flow limitA lower flow limit than PLAMaximum flow test
Part cooling fanOff for layer 1, then 100%Off for the first layers, then about 20 to 50%Overhangs and bridges
RetractionStock profile, often about 1 mm or less on direct drive and several mm on BowdenSame or slightly less, at a slower speedRetraction test

Resin printing basics

Most desktop resin printers (LCD and DLP) cure a whole layer at once with UV light, usually 405 nm, so print time depends on the tallest part, not on how many parts share the plate.

Layer height and exposure

Layers of 0.05 mm suit most parts, and 0.025 to 0.035 mm suits miniatures with fine faces. Exposure time is how long the screen lights each layer. Start from the resin maker's settings for your exact printer, since screens differ in power. As a rough guide, resin makers list about 2 to 3.5 seconds for normal layers of standard resin on mono LCD printers, and around 6 bottom layers at a much longer exposure, often 25 to 40 seconds, so the part bonds to the plate.

Then print an exposure test with pins, holes and fine features. Under-exposure loses thin pins. Over-exposure closes holes and bloats detail. Adjust in small steps and reprint.

Lift and temperature

After each layer the plate lifts to peel the cured layer off the vat film. Use the lift distance and speed in your printer or resin profile, and slow the lift for large cross-sections. Keep the resin and the room around 20 to 25 °C, the range resin makers commonly give. Cold resin is thick, cures poorly and fails.

Safety

  • Wear nitrile gloves, not latex, whenever you touch liquid resin, the vat or unwashed parts. Resin can cause an allergic skin reaction that worsens with repeated exposure. If it reaches skin, wash with soap and water, not alcohol.
  • Wear safety glasses when pouring resin or washing parts.
  • Print in a ventilated room nobody sleeps in, with the printer cover on, and check the resin's SDS for ventilation needs.
  • Wash parts in isopropyl alcohol (IPA) of 90% or stronger, often in two baths, dirty then clean, or in water for water-washable resin. IPA is highly flammable, so keep it sealed and away from heat, sparks and flames.
  • Dry parts fully, then cure them under 405 nm UV for the resin maker's time. Curing longer does not help and can yellow parts.
  • Never pour resin, used IPA or wash water down a drain or onto the ground. Cure leftover resin and resin-soaked wipes solid under UV, then dispose of them as the SDS and local rules require. Used IPA still holds dissolved resin, so ask your local waste service how to dispose of it.

Prepare the printer and start the print

  1. Clean the bed Wipe the cold plate with IPA of 90% or stronger. When wiping stops working, wash the plate in warm (not hot) water with a little dish soap and dry it fully. Hold plates by the edges, since skin oil ruins first-layer adhesion.
  2. Level or mesh the bed Most current printers probe the bed and build a height map, called a mesh. Rerun it after moving the printer or swapping plates. On a manually leveled printer, level at printing temperature.
  3. Set the Z offset The Z offset is the nozzle's gap above the bed on the first layer. Adjust it in 0.02 to 0.05 mm steps while the first layer prints.
  4. Dry hygroscopic filament PETG, TPU and nylon absorb moisture from the air, then pop, string and print weak. Dry them in a filament dryer at the maker's temperature, never in a kitchen oven used for food. The materials guide has typical drying settings.
  5. Check the spool Purge until the color runs clean and make sure the spool turns freely. A snag in the feed path starves the nozzle partway through a print.
  6. Watch the first layer Stay for all of it. The first layer decides whether the print succeeds.

What a good first layer looks like

Lines are slightly flattened and touch their neighbors with no gaps. Round lines with gaps between them mean the nozzle is too high, and the part will come loose. Thin, see-through lines with ridges mean it is too low. Fix it now with the Z offset rather than hoping later layers recover.

Monitoring the print

Check again after a few layers, then regularly. A camera helps, and some printers detect spaghetti failures and pause. Do not leave a printer running unattended, especially one with a heated bed, unless you have taken the fire precautions its maker recommends: a working smoke detector nearby, a non-flammable surface around the printer and thermal runaway protection (firmware that cuts the heaters when a temperature reading goes wrong) turned on.

Remove and finish the part

Let the bed cool, then flex the sheet to release the part, since pulling a part off a hot bed bends it. PETG can bond so hard to smooth PEI that it damages the sheet, so print it on textured PEI or use glue stick as a release layer.

Supports

Use flush cutters, needle-nose pliers and a deburring tool on FDM supports, and wear safety glasses, since snapped supports fly. Many hobby users remove resin supports, gloves on, after washing and before curing, when the tips snap off cleanly. Formlabs advises leaving them on through post-curing for most parts so thin features do not warp, so follow your resin maker.

Sanding

Start at 120 to 220 grit depending on the layer lines, move through 320 and 400, then wet sand up to 600 to 1000 grit for a smooth or glossy finish. Wet sanding also keeps dust down, and a dust mask is wise for dry sanding. Keep power tools slow, since friction softens PLA and smears it.

Filler primer and paint

Filler primer is a thick spray primer that fills layer lines. Spray two or three light coats outdoors or in a well-ventilated space, following the can's directions, sand at 320 to 400 grit and repeat until the lines are gone. Then paint with acrylics or spray paint in thin coats and seal with a matte or gloss clear coat. Finishing 3D prints goes further.

Heat-set inserts

Heat-set inserts are threaded brass inserts melted into a printed hole. They give screws threads that survive repeated assembly.

  1. Size the hole Use the insert maker's hole diameter, usually a little under the insert's outer diameter, and make the hole slightly deeper than the insert.
  2. Heat the iron Fit an insert tip to a soldering iron set to the insert maker's temperature for your plastic. The tip burns skin instantly and melting plastic gives off fumes, so ventilate, keep the iron in its stand between inserts and work on a heat-proof surface.
  3. Press straight Place the insert with the iron or tweezers, never your fingers. Let the heat sink it in with light, straight pressure, and stop just short of flush.
  4. Seat it flat Press it flush with a flat piece of metal while the plastic is still soft, let it cool, then test it with a screw. Switch the iron off and unplug it as soon as you finish.

Resin wash and cure

Wash for the time the resin maker gives, split between the dirty IPA bath and the clean one. Dry the part completely, since leftover IPA can leave a white film. Cure it for the resin maker's time, turning it so every side gets light. Curing past that time does not add strength and can yellow the part.

Check the part

A print that looks fine can still be 0.3 mm too big to fit. Check every part that has to work with something else.

Measure with calipers

Digital calipers that read to 0.01 mm are enough. Measure critical dimensions in X, Y and Z. A well-tuned FDM printer usually holds about 0.1 to 0.2 mm on small features, and holes tend to print undersized. For a consistent error, calibrate flow first, then adjust the slicer's XY compensation, which grows or shrinks holes and outlines, in 0.05 mm steps.

Test the fit

Print a tolerance test with pegs and holes at gaps from 0.1 to 0.5 mm. As a starting rule on FDM, a gap of 0.1 to 0.15 mm between surfaces gives a press fit, 0.2 to 0.3 mm a sliding fit and 0.4 to 0.5 mm a loose fit. Test with the real screws, magnets or inserts too.

Look closely

Inspect under one bright light held at a low angle, which shows blobs, seams and support scars that overhead light hides. Weigh the part too. One that comes out noticeably lighter than the slicer's estimate is usually under-extruded.

Quality check for each part

  • Critical dimensions within your tolerance in X, Y and Z
  • Mating parts, screws, magnets and inserts fit as intended
  • No stringing, blobs or zits on visible faces
  • Top surfaces fully closed
  • Support scars cleaned up and seams on hidden edges
  • Color and finish match the reference part
  • Weight close to the slicer's estimate

3D print troubleshooting

Find the symptom, check the causes in order and change one thing at a time. The last three rows are resin problems.

Common FDM and resin print failures, likely causes and fixes
ProblemLikely causesFixes
Warping (corners lift)Plastic shrinking as it cools, drafts, a cool bed, sharp cornersEnclosure for ABS, ASA and nylon, hotter bed within range, 5 to 10 mm brim, rounded corners, no fan on early layers
Poor bed adhesionDirty bed, nozzle too high, cool bed, fast first layerClean the bed, lower the Z offset in 0.02 mm steps, rerun the mesh, slow the first layer
Stringing (hairs between features)Wet filament, nozzle too hot, too little retractionDry the filament, lower the temperature 5 °C at a time, run a retraction test
Under-extrusion (gaps, thin walls)Partial clog, wet or tangled filament, speed past the hotend's flow limit, worn extruder gearCheck the feed path, do a cold pull, slow down or lower the flow limit, calibrate flow
Over-extrusion (blobs, oversized parts)Flow too high, wrong filament diameter in the profile, nozzle too hotCalibrate flow, check the profile's filament diameter matches the spool (usually 1.75 mm), lower the temperature
Elephant's foot (bottom layers bulge)Nozzle too close on the first layer, bed too hotRaise the Z offset slightly, lower the bed 5 °C, use elephant foot compensation, chamfer bottom edges 0.5 mm
Layer shiftsNozzle hitting curled plastic, loose belts or pulleys, acceleration too highFix the curling, tension the belts, tighten pulley set screws, lower acceleration
Ringing or ghosting (ripples after corners)Vibration at high speed or acceleration, a loose frame, a wobbly tableRun input shaping calibration if the printer has it, slow the outer walls, tighten the frame, use a solid surface
Gaps in top layers (pillowing)Too few top layers, very low infill, weak coolingUse 0.8 to 1.0 mm of top skin, raise the infill, add cooling for PLA
Spaghetti (loose tangles of filament)Part came off the bed, a failed support, a mid-print clogFix adhesion, add a brim or supports, reorient tall parts, turn on failure detection
Nozzle clogsHeat creep in a hot enclosure, debris, too much retraction, abrasive filament in a brass nozzleCold pull, new nozzle, open the enclosure for PLA, less retraction, hardened nozzle for abrasive filament
Wet filament (popping, steam, rough surface)Spool left in humid air, especially PETG, TPU and nylonDry it, store it sealed with desiccant, print hygroscopic materials from a dry box
Resin print not sticking to the platePlate not leveled, low bottom exposure, cold resin, dirty plateRelevel, raise the bottom exposure, warm the room to about 20 to 25 °C, clean the plate with IPA (gloves on)
Resin layer separationUnder-exposure, fast lift, cold resin, worn vat film, weak supportsRaise the exposure a little, slow the lift, warm the resin, replace damaged film, add supports
Resin suction or cupping (cracks, blowouts)Hollow sections with no vent, cup shapes that seal against the filmAdd at least two drain holes, one close to the build plate, tilt the part, slow the lift

No printer? Order the print

You do not need a printer to get a part made. Independent print shops can print it and ship it to you. Prepare the file the same way: check the mesh, confirm the size in millimeters and pick a suitable material.

The material families are PLA, PETG, ABS, ASA, TPU, resin and nylon, and choosing one filters to shops that stock it. Print strength comes in three choices: display, functional and solid. A file is refused if no shop's printer bed can hold it, so split oversized parts first. Hardware such as magnets, screws, LED kits and wiring can be added where your shop stocks it. There is no minimum order, and volume pricing starts at 25 units.

Larger runs work differently. With production quotes, you set the brief once with the file, quantity, process, material and need-by date. Approved production shops reply with a firm per-unit price and a lead time, across FDM, resin (SLA and DLP) and SLS or MJF. Nothing is charged until you accept a quote.

Printing products to sell

One good print is a hobby. Fifty identical prints is production, and the difference is process.

Lock your profiles

Save a named slicer profile for each product, material and printer, such as phone-stand_PETG_printerA_v3, and keep the 3MF project with the product. Treat a new filament brand, nozzle or firmware update as a new version, and recheck the first part.

Run a first-article check

Before a batch, check one part completely: dimensions, fit with mating parts and hardware, finish, color and weight. Keep it as the reference sample and judge every later part against it.

Check every batch

Inspect every part, and measure the first and last part of each plate, since a slowly clogging nozzle shows up at the end. Use one filament lot per batch where you can, because colors drift between lots. Log failures and their causes so each price carries a realistic failure allowance.

Before you sell a printed product

  • Named, versioned slicer profile saved with the 3MF project
  • First-article part measured, fit-tested and kept as the reference
  • Failure allowance included in the price
  • Filament lot recorded for each batch
  • Packaging tested with a real part
  • Material and care notes ready for the listing, such as keeping PLA out of hot cars

Designing for other people to print? On Printlooper, many sellers can list the same design with different print shops, so your file gets printed on printers and profiles you never see. Design with generous tolerances. If you run a print farm, see how print shops work with Printlooper.

Frequently asked questions

How do I start 3D printing as a beginner?

Start with a printer that ships with tuned slicer profiles, a spool of PLA and a small test model. Use the stock profile at 0.2 mm layers, clean the bed and watch the first layer closely. Print a few simple parts before you change settings, then calibrate temperature and flow for each new filament. Learn mesh checks, orientation and supports next, since they cause many failures that are not first-layer problems.

Why won't my 3D print stick to the bed?

The usual causes are a dirty bed, a nozzle set too high, a bed that is too cool or a first layer printed too fast. Clean the cold bed with IPA or with warm water and dish soap, lower the Z offset in 0.02 mm steps until the lines look slightly flattened, rerun bed leveling and slow the first layer. For corners that lift later, add a brim and check the bed temperature.

How long does a 3D print take?

It depends on size, layer height, walls, infill and printer speed. A small bracket can finish in under an hour, while a full-size helmet can run for 12 hours or more on one printer. Your slicer shows an estimate before you print, and halving the layer height roughly doubles it. On LCD and DLP resin printers, time depends on the height of the tallest part rather than on how many parts share the plate.

Do I need supports for my 3D print?

On FDM printers, add supports under overhangs more than about 45 to 50 degrees from vertical and under bridges longer than your printer handles cleanly in a bridge test. Reorienting the part or adding chamfers in the design often removes the need. Resin prints almost always need supports, because each layer peels away from the vat film, and unsupported islands get pulled off the part.

How can I get something 3D printed without a printer?

Upload the file to an online print service and choose a material. On Printlooper you can upload an STL or 3MF without an account, pick the material, color and finish, and compare all-in prices from approved print shops. Independent shops print and ship to US addresses, and each shop sets its own production time. For larger runs, request production quotes instead.

Is resin 3D printing safe at home?

Only with care. Read the resin's safety data sheet, wear nitrile gloves and safety glasses, print in a ventilated room nobody sleeps in, and keep resin and IPA away from children, pets and flames. Never pour resin, used IPA or wash water down a drain, and dispose of waste as the SDS and local rules require. Uncured resin can cause a skin allergy that worsens with repeated exposure, so avoid all skin contact.

Further reading

Sources

No printer? Get the part made

Upload an STL or 3MF, pick a material, color and finish, and compare all-in prices from independent print shops that ship to US addresses.